1.Types of raw materials:
a. Chrome ore, Cr2O3≥40%, Cr203/FeO≥2.5,S<0.05%, P<0.07%, MgO and Al2O3 should not too much higher, Size 10-70mm.
Silica ore: SiO2>97 %: Al2O3<1%: Stable in heat, and without Mud, size 20-80 mm.
Feeding size: large size furnace 30~100 mm; small size furnace 25~60 mm
b.fix carbon of carbon deoxidizer>84%:ash<15%:S<0.6%, feeding size:3~20 mm。
2Raw materials consumption(Cr 66% around):
Chrome ore 1880~2200 kg/t
Coke 410~500 kg/t
Silica 85~95 kg/t
Electrode 20~25 kg/t
Power consumption 2800~3100 kw.h/t
Power consumption of other main equipments: 400 kw/t around
3.Main operation index:
Daily production: 92 T
Unit power consumption: 3000~3400Kw.h
Qualified rate : >92~95%
Cos∮: 0.81
4.Power consumption:
Melting process 2800~3100 kw.h/t
Cooling process 55 kw.h/t around
Smoke 250 kw.h/t
5.Gas cleaning:
Gas temperature 300~800℃(central area)
~200℃ (tapping area)
Gas density 3~5 g/Nm3 (central area)
1.5 g/Nm3 (tapping area)
6.Grade and content of HIGH CARBON FeCr:
Grade |
Content /% | |||||||||
Cr | C | Si | P | S | ||||||
Range | Ⅰ | Ⅱ | Ⅰ | Ⅱ | Ⅰ | Ⅱ | Ⅰ | Ⅱ | ||
≥ | ≤ | |||||||||
FeCr67C6.0 | 62.0-72.0 | 6.0 | 3.0 | 0.03 | 0.04 | 0.06 | ||||
FeCr55C600 | 60.0 | 52.0 | 6.0 | 3.0 | 5.0 | 0.04 | 0.06 | 0.04 | 0.06 | |
FeCr67C9.5 | 62.0-72.0 | 9.5 | 3.0 | 0.03 | 0.04 | 0.06 | ||||
FeCr55C1000 | 60.0 | 52.0 | 10.0 | 3.0 | 5.0 | 0.04 | 0.06 | 0.04 | 0.06 |